DRAM Buried-Wordline Film Stack

A DRAM buried-wordline film stack recesses the entire gate below the active-area surface instead of sitting on top of it, trading the planar geometry of the DRAM wordline film stack for a trench-gate structure that cuts gate-induced drain leakage and frees the surface for the bitline and storage-node contacts that land directly above it. Samsung, SK Hynix, and Micron all moved to this buried recessed-gate (bRKG) geometry once DRAM half-pitch dropped below roughly 30 nanometers, because a planar gate at that pitch could no longer suppress subthreshold leakage well enough to hold a cell's charge for a usable refresh interval; the fix is to etch the gate down into the silicon rather than deposit it on top, which lengthens the effective channel inside the trench without consuming any extra surface footprint. The resulting four-film recipe at this step is a silicon trench cut into the active-area moat roughly 900-1400 angstroms deep, a thin thermal or ISSG gate-oxide liner roughly 35-55 angstroms thick conformally grown on the trench walls, a TiN barrier and work-function layer roughly 20-40 angstroms thick deposited by ALD to set the gate's threshold voltage and block tungsten diffusion into the oxide, and a tungsten fill with bulk resistivity near 5-8 micro-ohm-centimeters that is recessed back below the active-area surface line and sealed under a silicon-nitride cap roughly 400-700 angstroms thick.

Active-area silicon, post-STI
isolated moat defined by the DRAM active-area film stack
Trench etch
anisotropic Si etch, 900-1400 Å deep, sets channel length
Gate-oxide liner growth
thermal or ISSG SiO2, 35-55 Å, conformal on trench walls
TiN barrier ALD
20-40 Å, sets threshold voltage, blocks W diffusion
Tungsten fill
CVD W, ~5-8 µΩ·cm, fills trench above the TiN liner
Recess etch-back
W pulled back below the active-area surface line
Nitride cap deposition
Si3N4, 400-700 Å, seals the recess for the contacts above

The entire point of pushing the gate below the surface is what the recess buys back above it. On the planar wordline covered separately, the gate stack occupies real surface height that the self-aligned bitline contact has to be etched around, and the nitride cap there has to survive that contact etch while still sitting at surface level; on the buried geometry, the gate, its TiN barrier, and its own nitride cap are all pulled down below the active-area surface line before the bitline-contact module even starts, so the contact etch sees a flat silicon-and-shallow-trench-isolation surface rather than a stack of raised gate films to clear. This is also why the channel is effectively longer at the same cell pitch than a planar gate could achieve: the current path now wraps down one trench wall, across the trench floor, and back up the other wall, which suppresses the short-channel effects that would otherwise force an unworkable tradeoff between threshold voltage and leakage as cells shrink. The TiN barrier is not optional filler between the oxide and the tungsten — tungsten reacts with silicon oxide at the temperatures used downstream in the flow, so without a continuous 20-40 angstrom TiN layer the fill would consume the gate-oxide liner it depends on for isolation, and TiN's own work function is what actually sets the threshold voltage rather than doping concentration the way it does in a polysilicon gate.

DRAM Buried-Wordline Film Stack, Recessed Gate the gate sits below the active-area surface line, wrapped by silicon on three sides active-area silicon active-area surface source/drain gate oxide liner, 35-55 Å TiN barrier, 20-40 Å W fill, ~5-8 µΩ·cm (recessed below surface) nitride cap, 400-700 Å ~900-1400 Å trench depth channel wraps the trench floor and both walls — longer effective channel, same surface footprint flat surface above the cap is what the bitline-contact etch sees next

None of this comes for free in process complexity, which is the real reason the planar wordline survived as long as it did. Cutting a trench, lining it with a conformal oxide, depositing a continuous ALD barrier on sloped sidewalls, filling it void-free with tungsten, and then etching that tungsten back to a controlled depth without damaging the oxide liner is a materially harder sequence than growing a flat gate stack and patterning it, which is exactly why foundries only adopted the buried geometry once planar gates ran out of leakage margin rather than as a day-one choice. Equipment vendors building this stack reflect that complexity split by step: Applied Materials and Tokyo Electron supply the trench etch and tungsten recess-etch-back tools where depth uniformity across the array is the controlling spec, ASM International supplies the ALD TiN barrier and gate-oxide liner tools where sidewall conformality inside a sub-30-nanometer trench is the hard problem, and Lam Research supplies the tungsten CVD fill and nitride-cap deposition tools where void-free fill at high aspect ratio is the yield-limiting step. Recess depth and TiN thickness are tracked as tightly as any spec in the DRAM front end for the same reason the dielectric thickness is tracked on the planar stack: too shallow a recess leaves gate material protruding into the bitline-contact module's etch path, and too thin a TiN layer lets tungsten attack the oxide liner it is supposed to protect, either of which shows up downstream as a refresh-time or sense-margin failure rather than a visible defect.

Read a DRAM buried-wordline film stack through a leakage-suppression lens, not a planar-gate-replacement lens: the trench depth sets the effective channel length, the oxide liner sets gate leakage, the TiN barrier sets both the threshold voltage and whether the tungsten fill stays chemically isolated from that liner, and the recessed nitride cap clears a flat surface for the contacts above — the same four material families as the planar DRAM wordline film stack, rearranged into a trench specifically to buy back the short-channel margin a surface gate ran out of, and handed off to the same bitline contact and DRAM bitline film stack that depend on either geometry switching cleanly without ever discharging the capacitor it was built to isolate.

Take DRAM buried-wordline film stack further