Post-Etch via Trench Ash Strip Clean

Once the dual-damascene via and trench etch lands on the cap, the freshly cut sidewalls and via bottom are not clean dielectric and copper — they are coated with etch byproduct polymer, a fluorocarbon-rich residue deposited by the same CxFy/CHF3/C4F8-based chemistry that cut the low-k IMD, plus whatever photoresist or hard-mask remnants survived the etch, and all of that has to come off before barrier/seed deposition without attacking the exposed low-k sidewalls or corroding any copper the via punched down onto. The industry-standard sequence runs a dry plasma ash first to strip the bulk of the polymer and any remaining organic hard mask, then a wet chemical clean to pull the thin residual film and ionic contamination the ash cannot reach, because neither step alone gets the via/trench surface clean enough for void-free barrier/seed coverage: ash alone leaves fluorine- and metal-containing residue in the via bottom that shows up later as high contact resistance, while wet clean alone cannot touch a polymer layer that thick without excessive dielectric attack or impractically long dip times. The two failure modes this step has to manage simultaneously are low-k sidewall damage — oxidizing or reducing plasma species pulling carbon out of a carbon-doped oxide (CDO) film and leaving it hygroscopic — and copper-bottom corrosion or galvanic attack wherever the via already punched through the etch-stop cap onto a prior Cu line, so the ash chemistry, the wet clean chemistry, and their order all get chosen around whichever risk dominates for a given via/trench geometry and exposed-Cu condition.

Via/trench etch complete
Sidewalls and via bottom coated with fluorocarbon polymer, resist/hard-mask remnants
Plasma ash
Bulk polymer removal
O2, H2/N2, or reducing plasma strips organic residue and photoresist
Low-k exposure window
Sidewall carbon depletion risk scales with ash time and oxidizing species
Wet chemical clean
Residual film removal
Dilute HF, semi-aqueous, or proprietary post-etch-residue remover pulls ionic/metallic contamination
Cu-bottom protection
Corrosion-inhibitor chemistry added when via punches through cap to prior Cu line
Inspect
SEM/CD-SEM sidewall check, k-value and contact-resistance monitors
Ready for barrier/seed
Clean, undamaged via/trench surface handed to PVD barrier/seed redeposition
O2 plasma ashH2/N2 forming-gas ashDilute HF wet cleanSemi-aqueous wet cleanProprietary residue remover
Primary roleFast bulk strip of photoresist and thick fluorocarbon polymerLower-damage bulk strip, favored once low-k is exposedRemoves thin oxide/residual film, dissolves fluorinated byproduct saltsRemoves polymer and particulates with less aqueous attack on exposed CuFormulated specifically to lift post-etch residue without touching CDO carbon or bare Cu
Low-k damage riskHigh — oxidizing O radicals deplete methyl (Si-CH3) termination, k can rise from ~2.5 toward 3.0+Low — reducing H2 chemistry avoids the oxidation pathway, the standard "damage-free" ashLow at typical <1% HF concentration and short dip, but repeated dips accumulate carbon lossLow to moderate, better than straight aqueous HF for exposed low-kLow by design, but efficacy and damage trade off against formulation cost
Cu-bottom corrosion riskLow — dry plasma does not directly attack exposed Cu absent halogen residueLow — reducing chemistry is generally Cu-compatibleModerate — bare HF can etch exposed Cu and barrier remnants without an inhibitor packageLow — semi-aqueous formulations commonly include Cu corrosion inhibitorsLow — inhibitor chemistry built in specifically for via-bottom Cu exposure
Residue removal effectivenessHigh for bulk organic/fluorocarbon polymerHigh for bulk polymer, slightly slower strip rate than O2High for thin ionic/fluoride residue, weak on thick polymerHigh for particulate and polymer, gentler overallHigh when matched to the specific etch chemistry's byproduct
Typical production useFirst-pass strip when no Cu is exposed at the via bottomDefault ash once low-k sidewall exposure or Cu-bottom exposure is a concernLegacy/simple flows, now mostly combined with an inhibitor additiveCommon pairing after H2-based ash on exposed-low-k, exposed-Cu viasIncreasingly standard combined ash+wet sequence at advanced low-k/Cu nodes
Post-Etch Ash and Clean: Two Risks, One Window Residue must clear before barrier/seed, without k-value damage or Cu-bottom corrosion Plasma ash step low-k IMD sidewall carbon depletion at exposed sidewall residual polymer Wet clean step low-k IMD sidewall SiN/SiCN cap Cu line below corrosion-inhibitor film k-value shift with ash damage pristine CDO k≈2.5 H2-based ash k≈2.6-2.7 O2 overash k≥3.0 Cu-bottom corrosion risk with inhibitor H2 ash only bare HF dip O2 ash clears residue fastest but risks the largest k-value shift; H2-based ash plus an inhibited wet clean is the damage-mitigated default Dilute HF below ~1% concentration with a corrosion-inhibitor package lifts residual film without attacking via-bottom Cu Carbon-doped low-k films such as Black Diamond-class OSG are the most ash-sensitive dielectric in this step

The low-k damage mechanism at the center of this step is carbon depletion: carbon-doped oxide films such as Black Diamond-class OSG rely on Si-CH3 methyl termination to keep their dielectric constant low, and an oxidizing ash — straight O2 plasma in particular — strips that methyl termination from the exposed sidewall, leaving a porous, now-hydrophilic surface that absorbs atmospheric moisture and pushes the local k-value up from a pristine ~2.5 toward 3.0 or higher in the damaged skin layer, which is exactly the capacitance and leakage penalty the low-k film was deposited to avoid. H2/N2 forming-gas and other reducing ash chemistries were developed specifically as "damage-free" alternatives because they strip the fluorocarbon polymer and resist without the oxidizing radicals that drive carbon depletion, typically holding the sidewall k-shift to a few tenths rather than the half-point-or-more jump seen after an aggressive O2 overash; the trade-off is a slower strip rate, so production flows often still use a short O2 or mixed-chemistry step for the thickest polymer followed by a damage-minimized reducing finish. The wet clean that follows carries its own version of the same risk, since dilute HF at too high a concentration or too long a dip time can etch into an already carbon-depleted sidewall and widen the via or trench CD, which is why production recipes hold HF concentration under roughly 1% and increasingly favor semi-aqueous or proprietary post-etch-residue removers formulated to pull fluoride and metal-ion residue while leaving both the low-k carbon skeleton and any exposed Cu at the via bottom untouched.

Low-k Sidewall Damage: Carbon Depletion and k-Value Shift Methyl (Si-CH3) loss during ash turns a hydrophobic low-k skin hydrophilic Pristine CDO sidewall CH3CH3CH3 CH3CH3CH3 Intact methyl termination repels moisture k ≈ 2.5 Ashed / damaged sidewall OHOH2O OHOH2O Carbon-depleted, porous skin absorbs moisture k ≥ 3.0 oxidizing ash (O2 plasma) H2/N2-based "damage-free" ash chemistry limits this shift to a few tenths instead of the 0.5+ jump shown here

This ash-strip-clean step is the direct handoff from via-etch-stop-dual-damascene-integration: the via and trench geometry that etch defined now has to reach barrier/seed redeposition with its sidewalls dielectrically intact and its via-bottom Cu, where exposed, free of both residue and corrosion, or the next level inherits a contact-resistance or leakage problem baked in before a single barrier atom is deposited. The low-k damage risk this step manages is the same risk osg-process and airgap-process were built to avoid in the first place — a carbon-depleted, moisture-absorbing sidewall skin undoes exactly the k-value reduction those integration schemes spent a deposition step achieving, so a damage-mitigated ash-and-clean sequence is not optional polish but the only thing standing between a low-k dielectric stack on paper and a low-k dielectric stack that still measures low-k after etch. With the via/trench surface clean and the carbon skeleton preserved, the process hands off to barrier/seed PVD redeposition, where a thin Ta/TaN barrier and Cu seed layer go down on exactly the surface this step was responsible for protecting.