GAA Dummy Gate Removal
Removing the dummy gate is the one GAA process step whose entire job is to destroy something precisely, without damaging anything touching it. By the time this step runs, the dummy gate material (described structurally in this site's GAA dummy-gate film stack article and patterned by the process in this site's GAA dummy-gate patterning process article) has already done its job — holding the gate trench open through source/drain epitaxy growth and interlayer-dielectric (ILD) fill — and now has to come out completely, leaving a clean, empty trench with the nanosheet stack still sitting inside it, ready for the SiGe-release etch described in this site's gate-all-around-gaa-nanosheet-channel-release-process article. The constraint that makes this hard isn't removing the dummy material; it's removing it without touching the gate spacers, the source/drain epitaxy, or the ILD that are all now pressed directly against it.
Selectivity, not etch rate, is the number that matters here. A dummy-gate removal etch that simply strips amorphous silicon or polysilicon fast is useless if it also attacks the SiN or SiBCN gate spacer lining the trench sidewall, or pits the exposed silicon or SiGe source/drain epitaxy at the trench bottom, or erodes the ILD oxide surrounding the whole structure. Fabs target selectivity ratios on the order of 50:1 or higher — dummy-material removal rate versus spacer/epi/ILD removal rate — using a wet etch (commonly a TMAH-based or ammonia-peroxide wet chemistry for a-Si/poly against oxide and nitride) or a highly selective dry etch tuned specifically for this interface. A selectivity shortfall here doesn't show up as a visible defect immediately; it shows up later as elevated parasitic capacitance (from a thinned spacer) or elevated source/drain contact resistance (from pitted epi), both of which get diagnosed as "mysterious" device-level variation unless the fab traces it back to this specific removal step.
The trench geometry left behind inherits every upstream tolerance, with no room to correct for it here. Because the dummy gate was patterned to a tight CD budget (covered in the dummy-gate patterning article) and the spacers were deposited conformally against it, the empty trench after removal is effectively a cast of the dummy gate's exact shape — any CD or sidewall-angle error from the patterning step reappears unchanged in the trench the replacement-metal-gate fill has to occupy. This is also the step where the nanosheet stack, sitting at the bottom of the newly opened trench, becomes accessible to wet chemistry for the first time since source/drain epi — meaning any residue, native oxide, or incomplete removal at the trench bottom directly interferes with the SiGe-release etch that has to run immediately afterward.
The removal chemistry choice also has to respect what's underneath, not just what's beside it. Because the nanosheet stack sits directly below the dummy gate, any removal chemistry aggressive enough to leave residue or micro-pitting at the trench floor hands that defect straight to the SiGe-release etch that runs next — a step that already depends on a clean, well-defined Si/SiGe interface to selectively pull the SiGe layers out without damaging the Si channels. Fabs typically split this into two sub-steps: a bulk strip that clears the majority of the a-Si or poly quickly, followed by a slower, more selective finishing etch calibrated to stop cleanly at the nanosheet surface rather than drive straight through it. Tokyo Electron's and Lam Research's wet-clean and selective-etch platforms are both qualified for this two-stage approach on current 3nm-class and 2nm-class GAA lines specifically because a single aggressive strip step can't hit both the speed and the surface-quality targets at once.
Read dummy-gate removal not as a cleanup step but as the process that determines whether every upstream investment — the patterned gate length, the grown source/drain epitaxy, the filled ILD — survives intact into the replacement-metal-gate module, because a selectivity failure here erases margin that nothing downstream in the GAA flow can rebuild.